Under fluoroscopy, most of an interventional device simply disappears. Polymer shafts, balloons and stent struts are close to radiolucent, and the only structures the physician can see clearly are the small platinum-iridium rings at the working end of the catheter. Those marker bands are the reference points for lesion alignment, balloon landing and stent coverage, which makes them one of the few components where a tolerance measured in microns has a direct clinical consequence.
Pt90Ir10 — 90 percent platinum and 10 percent iridium by weight — has been the default marker alloy in vascular devices for decades. This guide explains why the alloy is so widely used, how the rings are specified, which standard sizes fit 0.014″, 0.018″, 0.035″ and structural heart systems, and what to check before an RFQ goes out.
What a marker band actually does
A marker band is a short cylindrical ring, usually 0.2–0.8 mm in axial length, cut from Pt-Ir tube and mounted on the device shaft — crimped onto a hypotube, bonded beneath a balloon, or welded at the proximal and distal ends of a stent. On the fluoroscope it appears as a dense, sharply defined bar. Four jobs depend on it:
- Lesion localisation. The rings bracket the target so the operator can place a balloon or stent against the lesion rather than against a guess.
- Length reference. Two markers with a known gap turn the screen into a ruler: pixel distance is converted to millimetres, which is how lesion length and stent coverage are judged.
- Deployment confirmation. When a balloon inflates or a stent foreshortens, the marker spacing changes. The operator reads that change as confirmation that the device behaved as intended.
- Tip visibility. A distal marker shows where the catheter actually sits in tortuous or heavily calcified anatomy, where the shaft itself gives no signal.
Why Pt90Ir10 is the default marker alloy
- Radiopacity. Platinum (Z = 78) and iridium (Z = 77) give the highest X-ray attenuation per unit wall thickness among the metals normally used for markers. A 0.030 mm wall is already clearly visible on standard fluoroscopy, so the ring can stay thin enough to fit inside a tight crossing profile.
- Biocompatibility. Pt-Ir is one of the oldest implant alloys in medicine — pacemaker electrodes and cochlear implants have used it for decades. It is chemically inert, releases no nickel, and its long clinical history makes the material system familiar to regulatory reviewers.
- Corrosion resistance. Both elements are noble. The alloy does not oxidise in saline or blood, does not pit, and does not shed ions into the surrounding tissue, so radiopacity and surface condition stay stable over the life of the device.
- Ductility and weldability. At the 90/10 ratio the alloy is ductile enough to be crimped or swaged onto a shaft by 10–20 µm of interference without cracking, and it can be welded or bonded into a delivery system without embrittling the joint.
- Stable, intrinsic visibility. There is no coating to flake and no contrast medium to wash out. The visibility comes from the bulk metal, so it cannot degrade during sterilisation, shelf life or repeated handling.
One practical caveat: any dense metal marker produces a local susceptibility artefact on MRI. Pt-Ir markers are intended for fluoroscopic visualisation, and the MRI labelling of the finished device remains the device manufacturer’s responsibility.
Where Pt90Ir10 marker bands are used
- Coronary stents and balloon catheters. 0.014″ ID, wall 0.030–0.050 mm, band width 0.25–0.40 mm. Drug-eluting stents typically carry two markers at each end so foreshortening can be read directly.
- Peripheral vascular devices. 0.018″ to 0.038″ ID with thicker walls (0.050–0.080 mm) for sheath, thrombectomy, stent and IVC filter delivery systems, where contrast has to survive a much larger vessel and a longer working distance.
- Neurointerventional microcatheters. 0.010″ to 0.018″ ID with walls of only 0.015–0.030 mm. Here the constraint is the microcatheter outer profile, so thin walls and short bands matter more than absolute brightness.
- Structural heart and electrophysiology. 0.042″ to 0.064″ ID, band widths of 0.50–0.80 mm and walls up to 0.12 mm, because the marker has to stay visible through the chest wall and diaphragm during occluder or lead delivery.

Between those four families the outside diameter moves from about 0.30 mm to 2.00 mm, which is why the same alloy arrives on a drawing as ten different parts rather than one.
Specifying a marker band: the four dimensions that matter
Almost every marker band problem traces back to one of four dimensions being specified loosely — or to the two properties nobody puts on the drawing.
| Dimension | What it controls | Typical drawing tolerance |
|---|---|---|
| Inner diameter (ID) | Fit on the hypotube or shaft, and the crimp interference that holds the ring in place | ±0.0005″ (approx. ±0.013 mm) |
| Outer diameter (OD) | Crossing profile of the finished device, and how much metal the X-ray beam passes through | ±0.0005″ (approx. ±0.013 mm) |
| Wall thickness | (OD − ID) / 2. Trades visibility against profile and sets crimp strength | ±0.002 to ±0.005 mm |
| Band width (axial length) | Visible length of the marker, and how precisely a lesion edge can be judged | ±0.05 mm |
| Concentricity / straightness | Uniform wall after crimping; an oval ring reads as a blurred marker | 0.01 mm |
| Edge condition | Burr-free, square-cut ends; burrs scratch balloons and block assembly | visual + 10× magnification |
Rule of thumb: ID usually sits 0.005–0.020 mm above the shaft diameter at that point, so the ring can be slipped into position and then crimped, swaged or bonded. If the application is adhesive-bonded rather than crimped, the clearance is taken from the adhesive thickness instead of from interference.

A drawing that calls all four of these critical cannot be met as a closed stack. Pick the two that decide whether the device works — usually ID and wall — and leave the rest as reference, which is the same advice the guide to marker band dimensions gives for any band, in any alloy.
Standard size reference by catheter system
The table below covers the ranges we cut most often. Inch figures are the nominal catheter system used on drawings; all other dimensions are in millimetres. Pt90Ir10 is the default material throughout.
| System | Nominal ID | ID (mm) | OD (mm) | Wall (mm) | Band width (mm) |
|---|---|---|---|---|---|
| Neuro microcatheter | 0.010″ | 0.254 | 0.300–0.330 | 0.015–0.022 | 0.20–0.25 |
| Neuro / intracranial | 0.014″ | 0.356 | 0.410–0.440 | 0.020–0.030 | 0.25–0.30 |
| Coronary PTCA / DES | 0.014″ | 0.356 | 0.420–0.460 | 0.030–0.050 | 0.25–0.40 |
| Small-vessel coronary | 0.016″ | 0.406 | 0.480–0.520 | 0.030–0.050 | 0.25–0.30 |
| Peripheral / neuro | 0.018″ | 0.457 | 0.530–0.580 | 0.025–0.035 | 0.30–0.40 |
| Peripheral balloon / stent | 0.025″ | 0.635 | 0.730–0.790 | 0.040–0.060 | 0.30–0.50 |
| Peripheral sheath / IVC filter | 0.035″ | 0.889 | 1.00–1.10 | 0.050–0.080 | 0.30–0.50 |
| Large access sheath | 0.038″ | 0.965 | 1.08–1.18 | 0.050–0.080 | 0.50 |
| Structural heart (ASD / LAA) | 0.042″ | 1.067 | 1.20–1.30 | 0.060–0.10 | 0.50–0.70 |
| Structural heart, large bore | 0.064″ | 1.626 | 1.82–2.00 | 0.080–0.12 | 0.50–0.80 |
Where a drawing already carries a reference part number instead of a size, the marker band cross-reference table maps those numbers onto the sizes above, so the first step of a quote is a lookup rather than a measurement.
A seven-point checklist before you send an RFQ
- Shaft diameter at the marker position. Measure the actual hypotube or shaft OD, not the nominal value. The ID follows from it plus the assembly clearance.
- Maximum outer profile allowed. This fixes the OD ceiling. On neuro and coronary devices the profile budget is usually the binding constraint, not radiopacity.
- Radiopacity actually required. Thin walls are often bright enough. Check the marker on the fluoroscopy system and setting the customer really uses before specifying a thicker wall.
- Number of bands and their spacing. Two markers with a defined gap give the operator a length scale; a single marker only gives a point. State the gap and its tolerance.
- Assembly method. Crimp or swage needs annealed ductility; adhesive bonding needs a clean, degreased surface; welding needs compatible metallurgy and a joint design that will not embrittle.
- Sterilisation and cleaning. Ethylene oxide, gamma and e-beam do not change Pt-Ir, but residual cutting oils and loose particles do matter. State the cleaning and packaging requirement.
- Documentation. Material certificate with alloy composition, dimensional inspection report, first article inspection for new drawings, and lot traceability.
What “precision” should mean in practice
Laser cutting is the standard route for these rings because it leaves a clean, square edge and no mechanical distortion of the tube. What separates a good marker band from an average one is usually invisible on a datasheet:
- Edge quality. A 10 µm burr inside a 0.35 mm ring is enough to scratch a balloon during assembly or to block the ring from sliding onto the shaft. Burr-free, square-cut ends should be specified and verified, not assumed.
- Wall concentricity. An eccentric wall makes one side of the marker brighter than the other and changes crimp behaviour around the circumference.
- Surface cleanliness. Cut rings must be degreased and free of embedded abrasive or loose particles before they enter a cleanroom assembly line.
- Dimensional verification. ID, OD and width checked by optical or pin gauging, either 100 percent or on a defined AQL sampling plan, with results traceable to the lot.
- Handling and packaging. Rings are easily deformed. Packaging that keeps them separated and undistorted protects the tolerance you paid for.
Custom sizes, finishing and OEM / ODM
Because the rings are cut from Pt-Ir tube to a drawing rather than produced from dedicated tooling, custom inner diameter, outer diameter, wall thickness and band width are straightforward — including sizes that fall between the standard rows above. We also support tighter tolerance bands, alternative edge and surface finishing, special packaging, and quantities anywhere from prototype lots to production releases.
For a quotation, send a drawing (PDF or DXF) with material, all dimensions and tolerances, band width, quantity, assembly method and target application. If a dimension is flexible, say so — it is often the difference between a fast, economic part and an over-specified one. OEM and ODM enquiries are welcome, and we can work to your drawing under NDA. The custom marker bands page covers the cutting, deburring and inspection route in more detail.
Tantalum and gold: when to deviate from Pt90Ir10
Pt90Ir10 is the default because it balances visibility, strength and cost. Two alternatives are worth knowing:
- Tantalum. Lower cost, but at 16.65 g/cm³ it needs about 30 percent more wall than Pt-Ir for the same contrast, and the metal is less ductile. A reasonable choice for cost-sensitive peripheral catheters where profile is not critical.
- Gold. The softest and easiest to crimp, which makes it popular for guidewire tips and very small markers. It is also the weakest under balloon pressure and the most expensive of the three.
Pure platinum sits between them: excellent ductility and radiopacity, but soft and costly. Where a customer’s drawing already specifies Ta or Au, we cut those alloys to the same dimensional standard, and the relative wall thickness of all three is compared side by side in marker band materials.
Frequently asked questions
What does Pt90Ir10 mean?
90 percent platinum and 10 percent iridium by weight. The iridium raises hardness and strength compared with pure platinum, so the ring can be crimped without collapsing, while the platinum keeps radiopacity and corrosion resistance at implant grade.
Why not use pure platinum?
Pure platinum is soft enough to deform during crimping and assembly, and it is more expensive. The 10 percent iridium addition gives the alloy the mechanical stability a marker band needs without a meaningful loss of visibility.
Marker band or marker ring — is there a difference?
They are the same component. “Marker band” usually refers to the cylindrical ring itself, and “marker ring” is used interchangeably, especially for stent and occluder markers.
Can I order small quantities or a one-off size?
Yes. Standard sizes can be supplied in prototype and production quantities, and custom sizes are cut to drawing without dedicated tooling, so a new size does not require a large minimum order.
Are Pt90Ir10 markers MRI compatible?
Marker bands are specified for fluoroscopic visualisation. MRI compatibility depends on the finished device design, the marker mass and the labelling strategy, and has to be evaluated by the device manufacturer.
What information do you need to quote a custom marker band?
Send the shaft OD, maximum device OD, required band width, number of markers, assembly method, quantity and sterilisation route. With those six inputs we can usually propose a size and tolerance band from stock dimensions the same day.
Request Pt90Ir10 marker bands to your drawing
Standard sizes are available from stock, and custom Pt90Ir10 marker bands are laser-cut to your drawing with burr-free edges, controlled ID/OD and width tolerances, and lot-level dimensional reporting. Send your drawing or a short specification through the inquiry form and we will come back with a size recommendation, tolerance review and quotation — including advice on where a dimension can be relaxed to reduce cost without affecting performance.